Top 5 Nickel Alloys For High-Temperature Applications: A Temperature-Band Selection Matrix
Nov 24, 2026

Introduction
Furnace projects rarely fail on alloy choice alone. They fail when the grade is picked from a price list instead of a temperature band. Inconel 600 sags at 1150 °C where Inconel 601 does not, and Inconel 718, the strongest grade here, loses half its rupture life within 50 °C of its ceiling.
This guide ranks these five grades by the band in which each is the lowest-cost alloy that survives.
Product Overview
Inconel 600 (UNS N06600). Nickel 72% minimum, chromium 14–17%, no strengthening additions. Oxidation to about 1093 °C, excellent chloride stress-corrosion resistance, and the lowest price here. The default for furnace fixtures and sheaths at moderate duty.
Inconel 601 (UNS N06601). Chromium 21–25% plus 1.0–1.7% aluminium, which forms an Al2O3 subscale that re-forms after spalling. That is why 601 survives cycling to about 1200 °C where 600 fails: radiant tubes, retorts and annealing baskets.
Inconel 625 (UNS N06625). Chromium 20–23%, molybdenum 8–10%, niobium plus tantalum 3.15–4.15%. Minimum yield of 414 MPa, roughly double 600's, and molybdenum that keeps chlorides from pitting. The grade for hot duty that is also wet.
Inconel 718 (UNS N07718). Gamma-double-prime precipitation lifts minimum yield to about 1030 MPa and tensile strength past 1240 MPa. It dominates structural duty to 650 °C: turbine disks, shafts, fasteners and valve stems.
Hastelloy X (UNS N06002). A nickel–chromium–iron–molybdenum alloy with 20.5–23% chromium and 8–10% molybdenum. It holds usable stress-rupture strength from 870 to 1200 °C and resists carburizing and nitriding gas.
Compare the full range on our nickel alloys and Inconel alloy pages.
Comparison Table
Table 1 - Chemical composition (wt%, typical)
| Element | 600 (N06600) | 601 (N06601) | 625 (N06625) | 718 (N07718) | X (N06002) |
|---|---|---|---|---|---|
| Ni | ≥72.0 | 58.0–63.0 | ≥58.0 | 50.0–55.0 | balance |
| Cr | 14.0–17.0 | 21.0–25.0 | 20.0–23.0 | 17.0–21.0 | 20.5–23.0 |
| Fe | 6.0–10.0 | ≤18.0 | ≤5.0 | balance | 17.0–20.0 |
| Mo | - | - | 8.0–10.0 | 2.8–3.3 | 8.0–10.0 |
| Al | - | 1.0–1.7 | ≤0.40 | 0.20–0.80 | - |
| Ti | - | - | ≤0.40 | 0.65–1.15 | - |
| Nb + Ta | - | - | 3.15–4.15 | 4.75–5.50 | - |
| Co | - | - | ≤1.0 | ≤1.0 | 0.5–2.5 |
| C | ≤0.15 | ≤0.10 | ≤0.10 | ≤0.08 | ≤0.15 |
Table 2 - Physical and mechanical properties (annealed, room temperature)
| Property | 600 | 601 | 625 | 718 | X |
|---|---|---|---|---|---|
| Density (g/cm³) | 8.47 | 8.11 | 8.44 | 8.19 | 8.22 |
| Melting range (°C, approx.) | 1354–1413 | 1360–1411 | 1290–1350 | 1260–1336 | 1260–1355 |
| Expansion, 20–100 °C (μm/m·K) | 13.3 | 13.6 | 12.8 | 13.0 | 13.9 |
| Conductivity at 20 °C (W/m·K) | 14.8 | 11.2 | 9.8 | 11.4 | 9.1 |
| Tensile strength (MPa) | 550–655 | 600–700 | 827–930 | 1240–1280 | 690–760 |
| Yield strength, 0.2% (MPa) | 240–310 | 240–300 | 414–517 | 1030–1100 | 275–345 |
| Elongation (%) | 35–45 | 35–40 | 30–40 | 12–20 | 40–45 |
| Oxidation ceiling in air (°C) | ~1093 | ~1200 | ~980 | ~980 | ~1200 |
| Sustained-load ceiling (°C) | ~800 | ~900 | ~650 | ~650 | ~1000 |
Table 3 - Temperature-band selection matrix
| Band | First choice | Alternative | Elimination rule |
|---|---|---|---|
| 600–800 °C, clean air | 600 | 601 for cycling | 718 only if stress exceeds 400 MPa |
| 600–800 °C, chlorides or acids | 625 | - | 600 and 601 pit in wet chloride |
| 800–1000 °C, load-bearing | 625 | X for carburizing gas | 718 out: gamma-double-prime coarsens |
| 1000–1150 °C, oxidizing, cycled | 601 | X for mixed gas | 600 out: chromium too low |
| 1150–1200 °C, low load | X | 601 short-term | 625 out: oxidation limit ~980 °C |
| Above 1200 °C | none of these | ceramics, ODS alloys | All five creep out |
Performance Analysis
Oxidation and spalling
The ceiling is set by surface chromium activity and by whether the scale survives cooling. 600 holds a Cr2O3 scale to about 1093 °C in continuous service, but it spalls under cycling and each spall consumes chromium. 601 uses aluminium instead: a thinner Al2O3 subscale that re-forms in service. Hastelloy X reaches a similar ceiling through chromium plus a matrix that resists inward attack in combustion gas. 625 and 718 are rated near 980 °C.
Creep and structural load
Ranking by room-temperature strength misleads. 718 is the strongest grade here and the weakest above 700 °C, because its strengthening phase transforms to delta and rupture life collapses. Solid-solution grades trade peak strength for stability: 625 is normally limited to 650 °C under sustained load, while Hastelloy X keeps usable stress-rupture strength to about 1000 °C. Where creep sets wall thickness, the order runs X, then 601 and 625, then 600.
Atmosphere chemistry
Air is the easy case. Carburizing gas diffuses carbon inward, and Hastelloy X is the only grade here used routinely in carburizing and nitriding furnaces and reformer outlets. 601 handles oxidizing sulphur-free flue gas but suffers in reducing sulphur atmospheres. 600 suits vacuum fixtures and high-purity gas.
Fabrication and welding
600 and 601 form and weld most easily with ERNiCr-3 filler and low interpass temperature. 625 and X work-harden quickly, so machining needs sharp tools and heavy feed. 718 is welded annealed with ERNiFeCr-2 and aged afterwards; welding it aged risks strain-age cracking.
Application Guide
Heat treatment furnaces. Inconel 601 for radiant tubes, retorts, muffles and baskets cycled to 1200 °C; Hastelloy X for rolls, skid rails and fan blades in carburizing zones; Inconel 600 for lighter fixtures and sheaths below 1000 °C.
Aerospace and turbines. Inconel 718 for disks, shafts and fasteners governed by 650 °C strength; Hastelloy X for combustor liners and exhaust structures; Inconel 625 for ducting that needs fatigue plus corrosion resistance.
Chemical and power plant. Inconel 625 for heat exchanger tubing, reactor internals and bellows where heat meets chloride or acid; Inconel 600 for caustic evaporator tubes.
Procurement shortcut. Two questions decide the row: metal temperature at the hottest 100 hours, and what is in the gas or liquid.
FAQ
Which of these five works above 1100 °C?
Only 601 and Hastelloy X, and only at low load. In oxidizing, cycled duty 601. in carburizing gas, Hastelloy X. None is rated above 1200 °C continuous.
Why can Inconel 718 not be used at 800 °C despite its strength?
Its gamma-double-prime phase transforms to delta above about 650 °C, so stress-rupture life drops even though a short tensile test looks healthy. Above 700 °C, 625 or Hastelloy X are safer.
Can Inconel 601 replace 625 to save cost?
Only where the medium is clean and oxidizing. 601 has no molybdenum, so chlorides, acids and wet crevices attack it.
Is Inconel 600 still worth specifying?
Yes, below about 1000 °C in clean atmospheres, caustic service and vacuum furnaces. It is the cheapest grade here and its chloride SCC resistance beats 601's, but do not push it into cyclic duty near 1100 °C.
What filler metals match these grades?
ERNiCr-3 for 600 and 601, ERNiCrMo-3 for 625, ERNiCrMo-3 or ERNiFeCr-2 for Hastelloy X, and ERNiFeCr-2 for 718. Matching composition matters most in 625 and X, where dilution lowers molybdenum and creates a corrosion-prone weld bead.
Conclusion
Selection means finding the band, not the brand: 718 where 650 °C strength sets the section, 601 where cyclic oxidation near 1200 °C sets the life, 625 where heat arrives with chlorides, Hastelloy X where the atmosphere carburizes, and 600 for everything moderate and clean. All five grades are available from Hitemp Alloys in plate, sheet, bar, wire and tube - send your duty conditions to our technical team and we will confirm band and delivery form.